A solvent pump seal normally runs a carbon face against silicon carbide, and the O-ring is the bigger decision: its compound has to match the solvent family, because NBR fails in most solvents and standard FKM fails in ketones, esters and methanol.
Seal Faces for a Solvent Pump
A solvent pump needs a self-lubricating soft face running against a hard one, because a thin solvent, or one that flashes to vapor as it crosses the sealing gap, leaves the faces running in boundary or mixed lubrication. The solvent’s low viscosity and volatility drive this choice, not chemical attack on the faces.
Avoid alumina where the solvent can flash or the seal can run dry. High-purity alumina resists most solvents chemically, but it cracks under thermal shock.
Carbon Against Silicon Carbide or Hard Against Hard
Carbon against silicon carbide is the default for solvent service, as it is for any thin liquid the carbon can tolerate. Hard against hard is reserved for streams that carry solids, or for products where carbon is not allowed, such as a batch that carbon wear would discolor.
The carbon grade matters more than the pairing, because a low-viscosity solvent can blister a porous carbon face. Resin-impregnated carbon, the general-purpose grade, blisters more easily.
Antimony-impregnated carbon resists blistering better, but it is poor in acids and bases, where resin carbon handles strong acids to strong bases. For a light, volatile solvent, ask for the lowest-porosity, blister-resistant grade the carbon supplier offers, and confirm antimony carbon against anything acidic or alkaline in the stream.
When a hard pair is unavoidable on a thin or flashing solvent, graphite-loaded silicon carbide is the better hard face, at some cost in strength and abrasion resistance.
Which Silicon Carbide Grade
A clean solvent does not need sintered silicon carbide; reaction-bonded silicon carbide handles it.
Choose sintered silicon carbide when the stream, a reaction by-product or the cleaning-in-place chemicals can be strongly alkaline or strongly acidic. Otherwise stay with reaction-bonded: sintered silicon carbide lacks its rubbing behavior, which counts on a low-lubricity solvent.
O-Ring Compounds by Solvent Family
EPDM suits acetone, MEK and alcohols; FKM suits aromatics and most chlorinated solvents; FFKM suits all of them; NBR suits only aliphatic solvents such as hexane. Esters and the heavier ketones have no satisfactory choice short of FFKM or a specialty fluoroelastomer.
The table gives Parker’s ratings, from its O-Ring Handbook, for its sealing-grade compounds of each polymer. Satisfactory means suitable; Fair and Doubtful mean, in the maker’s words, usually or sometimes acceptable for a static seal only.
| Solvent | Family | NBR | EPDM | FKM (standard) | FFKM |
|---|---|---|---|---|---|
| Acetone | Ketone | Unsatisfactory | Satisfactory | Unsatisfactory | Satisfactory |
| Methyl ethyl ketone (MEK) | Ketone | Unsatisfactory | Satisfactory | Unsatisfactory | Satisfactory |
| Methyl isobutyl ketone (MIBK) | Ketone | Unsatisfactory | Doubtful | Unsatisfactory | Satisfactory |
| Cyclohexanone | Ketone | Unsatisfactory | Fair | Unsatisfactory | Satisfactory |
| Ethyl acetate | Ester | Unsatisfactory | Fair | Unsatisfactory | Satisfactory |
| Butyl acetate | Ester | Unsatisfactory | Fair | Unsatisfactory | Satisfactory |
| Toluene | Aromatic | Unsatisfactory | Unsatisfactory | Satisfactory | Satisfactory |
| Xylene | Aromatic | Unsatisfactory | Unsatisfactory | Satisfactory | Satisfactory |
| Benzene | Aromatic | Unsatisfactory | Unsatisfactory | Satisfactory | Satisfactory |
| Methylene chloride | Chlorinated | Unsatisfactory | Unsatisfactory | Fair | Satisfactory |
| Trichloroethylene | Chlorinated | Doubtful | Unsatisfactory | Satisfactory | Satisfactory |
| Chloroform | Chlorinated | Unsatisfactory | Unsatisfactory | Satisfactory | Satisfactory |
| Methanol | Alcohol | Unsatisfactory | Satisfactory | Unsatisfactory | Satisfactory |
| Ethanol | Alcohol | Doubtful | Satisfactory | Doubtful | Satisfactory |
| Isopropyl alcohol | Alcohol | Fair | Satisfactory | Satisfactory | Satisfactory |
| Hexane | Aliphatic | Satisfactory | Unsatisfactory | Satisfactory | Satisfactory |
A Fair rating is not enough for the O-ring that slides on the sleeve of a pusher seal. That rules out EPDM in esters and standard FKM in methylene chloride for the dynamic position.
Specialty fluoroelastomer grades made to resist low-molecular-weight ketones and esters have to be ordered by grade name, since “FKM” or “Viton” on a drawing does not specify one.
When to Use FFKM or PTFE Instead
Use FFKM when no lower-cost elastomer is rated satisfactory for the dynamic O-ring, or when the pump sees more than one solvent family.
Producers make several FFKM compounds tuned for different chemicals and temperatures, so the order should name the compound selected for the actual fluids and temperature.
PTFE is the option when even FFKM is in doubt, since very few chemicals attack it. In a mechanical seal it appears as spring-energized wedges, as bellows or as gaskets, and wedges can hang up in dirty service, fret the shaft sleeve and allow only limited axial movement. API 682 excludes wedge designs.
FEP- or PFA-encapsulated O-rings put a fluoropolymer jacket over an FKM or silicone core. They suit the static positions, such as the stationary seat O-ring and the gland gasket, but not the dynamic O-ring.
The elastomer-free route is a seal without a sliding O-ring. A metal bellows seal, a non-pusher design, replaces the dynamic O-ring with a formed or welded bellows, leaving only static seals to choose.
Why the Solvent Name Is Not Enough
A compound has to suit every fluid that touches the seal at the temperature it actually sees, and the solvent name covers only one of them. Flush liquids, lubricants and cleaning fluids count as process fluids for the O-ring.
Temperature shifts every rating: a borderline rating at room temperature can become a failure at process temperature.
Mixtures need the same care: a stream of toluene with some acetone needs a compound that suits both, which often leaves only FFKM.
Two O-rings sold as the same polymer can behave differently in the same solvent. Compatibility tables are a starting point, and the selected compound should be proven under actual service conditions.
A removed O-ring that is swollen, cracked or hardened shows the compound did not suit the stream, one of the common causes of O-ring failure in mechanical seals.