A sulfuric acid pump needs a seal matched to the acid’s concentration and temperature: sintered silicon carbide faces, a secondary seal and spring metal rated for that concentration band, and an external PTFE bellows seal or a double seal where the duty calls for one.

Three substitutions are the common traps on this service: reaction-bonded silicon carbide in place of sintered, a general-purpose FKM O-ring, and 316 stainless springs in mid-strength acid.

How Concentration and Temperature Change the Seal

Concentration sets which kind of attack the seal sees, and temperature sets how fast it goes. Sulfuric acid at about 40–60 % is a strong reducing acid: stainless steel cannot keep its passive film there, and with chlorides in the acid even high-nickel stainless grades such as 904L do not resist that 40–60 % range.

Above about 90 %, sulfuric acid turns oxidizing, which is extremely aggressive when the acid is impure. Below about 20 %, several stainless grades can be suitable even with significant chlorides present.

Corrosion rate generally rises with temperature. Small swings in strength matter as much as the nominal grade, so specify the concentration as a range that includes upsets and start-up dilution.

To quote a seal for this service, a supplier needs the concentration range, the temperature range, chloride and other impurity content, any solids, seal chamber pressure and shaft speed. For a replacement chemical pump seal, add the existing seal’s drawing, its part number or the old seal itself as a sample.

Seal Faces for Sulfuric Acid

Sintered silicon carbide is the face material for sulfuric acid, run against itself or, in weaker acid, against carbon. Reaction-bonded SiC and cobalt-bound tungsten carbide look like equivalents on a drawing, but both corrode far faster than sintered SiC in hot concentrated acid.

Saint-Gobain’s immersion test of face materials in 98 % sulfuric acid at 100 °C shows the gap:

Face material as testedWeight loss in 98 % sulfuric acid at 100 °C (mg/cm²·yr)Saint-Gobain’s service guide for that rate
Sintered SiC, no free silicon (Hexoloy SA)1.8Recommended for long-term service
Reaction-bonded SiC, 12 % silicon55.0Not recommended for service greater than one year
Alumina, 99 %65.0Not recommended for service greater than one year
Tungsten carbide, 6 % cobalt>1000Completely destroyed within days

So when a drawing says only “SiC”, confirm the sintered or reaction-bonded grade before the seal goes into concentrated acid. A tungsten carbide face with a cobalt binder has no place on this duty.

No published limit covers carbon seal-face grades in concentrated acid, so run sintered SiC against sintered SiC above about 85 %.

Where carbon does go into weaker acid, the impregnant matters. Resin-impregnated grades are made for mild chemical solutions, and carbon-impregnated grades for highly corrosive environments.

O-Ring Materials for Sulfuric Acid

PTFE and FFKM resist sulfuric acid across the concentration range. FKM holds in concentrated acid only in a compound rated for it, and EPDM belongs in dilute acid.

The letters FKM alone do not define acid resistance: standard bisphenol-cured FKM grades are poor against acids and peroxide-cured grades excellent. Parker’s O-ring compatibility table, for its recommended compounds, rates the common elastomers in sulfuric acid as follows (1 satisfactory, 2 fair, 3 doubtful, 4 unsatisfactory, X insufficient data):

Elastomer3 molar acid, to 70 °CConcentrated acid, room temperatureConcentrated acid, to 70 °C
Nitrile (NBR)2X4
EPDM134
FKM111
FFKM111

Parker’s FKM rating of 1 in concentrated sulfuric acid applies to its own recommended compound and stops at 70 °C. Ask for the compound and its acid rating before fitting FKM in concentrated acid, even where a general compatibility chart lists FKM for sulfuric acid.

Above 70 °C in concentrated acid, the choice is FFKM or PTFE, and FFKM varies by compound as well.

Seal Spring and Hardware Metals for Sulfuric Acid

316L springs and hardware are safe only in cold acid at the two ends of the concentration range; in mid-strength or hot acid the metal has to be a nickel alloy used inside its temperature limit, or kept out of the acid altogether. Corrosion tables treat a loss of 0.1 mm a year as acceptable for continuous exposure, which suits a pipe wall. A spring of thin wire has far less metal to lose, so a material sitting near that line is not a spring material.

  • 316L: Alleima rates its 316L-type grade 3R60 corrosion-proof (under 0.1 mm/year) in 94–98 % sulfuric acid up to 40 °C, and not usable (over 1.0 mm/year) in 40–70 % sulfuric acid even at 20 °C. That grade carries about 2.6 % molybdenum, more than ordinary 316L, so treat those limits as the best case.
  • Alloy 20: developed for sulfuric acid, Alloy 20 is the step up from 316 in dilute and mid-range acid, though even Alloy 20 exceeds 0.1 mm/a in boiling acid.
  • Hastelloy C-276: Haynes’ reagent-grade data put C-276 under 0.1 mm/y at 66 °C in 50–90 % sulfuric acid, and over 0.1 mm/y at 93 °C at every concentration listed, so check the temperature before specifying C-276 hardware for hot concentrated acid.
  • Titanium: not an upgrade on this service. One steel producer’s sulfuric acid table rates commercially pure titanium not usable (over 1.0 mm/year) at every concentration from 20 % to 98 %.

External PTFE Bellows or Internal Seal

Use an external PTFE bellows seal when no spring or hardware metal holds up in the acid at the duty’s concentration and temperature, and the duty stays inside the bellows’ temperature and pressure limits.

Check the temperature, pressure and speed limits on the manufacturer’s data for the PTFE bellows seal you are fitting. Read the pressure limit at the duty temperature, not at room temperature, because a PTFE bellows holds less pressure as it gets hotter.

Acid duties hotter than the bellows’ rated temperature take an internal seal with sintered SiC faces, FFKM or PTFE secondary seals, and springs or a metal bellows in an alloy proven for that concentration and temperature. Where the duty runs hotter than every alloy figure in the previous section, that proof has to come from the plant’s own corrosion data.

Single or Double Seal

Sulfuric acid service needs a double seal wherever the site cannot accept acid leaking to atmosphere; a single seal fits only where small leakage can be contained and controlled. API 682 bases the choice on how hazardous leakage is:

  • Single seal (Arrangement 1): for fluids whose leakage is not critical or can easily be controlled.
  • Unpressurized dual seal (Arrangement 2): captures leakage across the inner seal for disposal, though small amounts can still reach atmosphere.
  • Pressurized dual seal (Arrangement 3): a barrier fluid held above seal chamber pressure prevents process leakage, for duties where no leakage is allowed.

The site’s own hazard assessment for its acid sets the arrangement.

Where no seal leakage path is acceptable at all, the alternative is a sealless magnetic drive pump.

Which Flush or Barrier Fluid to Use

No barrier or flush fluid is safe with sulfuric acid by default: it must not react with the acid, and it must be acceptable as a contaminant in it. Water is safe only against acid below about 80 % strength.

A single seal flushed from the pump’s own discharge circulates the acid itself, so the question arises only when an outside fluid enters the seal chamber: an external flush, a quench or a double seal’s barrier.

In a pressurized barrier system such as Plan 53A or Plan 54, barrier fluid leaks into the process in normal operation, and much more of it enters if the inner seal fails. Choose a barrier the acid and the downstream process can absorb at that failure volume. Glycol–water mixtures, the common general-purpose barrier, still carry water into the acid.